Researchers synthesized manganese-doped CdSe/CdS quantum dots, fabricated them into photoconductive Auston-switch devices, and characterized their optical and electrical behavior using transient-absorption (TA) and time-resolved photocurrent (TPC) measurements. The procedures involved preparing wurtzite CdSe cores, incorporating approximately two to five Mn2+ ions per quantum dot through diffusion doping, coating the cores with CdS shells, and assembling the dots into a gold-electrode device on a glass substrate.
Materials
Cadmium oxide (CdO, 99.99%, Aldrich), octadecylphosphonic acid (ODPA, 99%, PCI), trioctylphosphine oxide (TOPO, 99%, Aldrich), trioctylphosphine (TOP, 97%, Aldrich), diphenylphosphine (DPP, 98%, Aldrich), selenium (Se, 200 mesh, 99.999%, Alfa Aesar), 1-octadecene (ODE, 90%, Aldrich), oleic acid (OA, 90%, Aldrich), oleylamine (OAm, 70%, Aldrich), manganese(II) acetate tetrahydrate (Mn(CH3COO)2·4H2O, 99.999%, Strem), and tributylphosphine (TBP, 95%, Aldrich) were used as received.
Synthesis of Mn-doped core/shell CdSe/CdS quantum dots
CdSe core synthesis
CdSe core particles with a wurtzite crystal structure were synthesized according to a previously reported method.17 CdO (100 mg), ODPA (490 mg), and TOPO (5 g) were placed in a three-necked flask and degassed at 150 °C for 1 hour under vacuum. Under a nitrogen stream, the mixture was heated to 320 °C and held at that temperature until a clear solution formed. TOP (1 ml) was then rapidly injected into the flask. After the temperature reached 380 °C, 1 ml of a 1.4 M TOP-Se solution was rapidly injected. At this stage, DPP was added to the TOP-Se solution at 1 mol% to control the growth rate.17 After 3 minutes, the heating mantle was removed and the reaction mixture was cooled to room temperature.
The resulting nanocrystals were collected by adding ethanol and centrifuging at 8,000 rpm. The washing procedure was repeated three times. The purified nanocrystals were then redispersed in toluene.
Mn doping
A diffusion-doping procedure was used to incorporate Mn into the synthesized CdSe nanocrystals.16 The protocol followed the procedure described in Ref. 17 To remove residual Cd species, presynthesized CdSe nanocrystals dispersed in toluene were precipitated with ethanol. A 75 mg portion of the precipitate was dissolved in a mixture of 27 ml of degassed ODE and 2.7 ml of OA. The mixture was heated to 60 °C under vacuum for 1 hour. After cooling to room temperature, the nanocrystals were again precipitated with ethanol and collected by centrifugation at 8,000 rpm. The resulting precipitate was added to a mixture containing Se (510 mg), degassed ODE (3 ml), and TBP (3 ml).
Separately, manganese(II) acetate tetrahydrate (90 mg), ODE (45 ml), OA (1.8 ml), and OAm (3.9 ml) were placed in a flask and degassed under vacuum at 100 °C for 1 hour. Under a nitrogen flow, the mixture was heated to 300 °C, after which the preprepared ODE solution containing the CdSe nanocrystals and TBP-Se was rapidly injected. The reaction temperature was maintained at 300 °C, and the doping level was controlled by the reaction time, typically 5–30 minutes. The mixture was then cooled to room temperature.
Magnetic circular dichroism measurements indicated that the quantum dots contained approximately two to five internal Mn2+ dopants per quantum dot, depending on the doping time.17
Growth of the CdS shell
Because of their large number of surface trap states, the as-prepared Mn-doped CdSe cores did not show detectable photoluminescence. To suppress surface defects, the cores were coated with a CdS shell using the procedure reported in Ref. 17
To prepare the Cd oleate precursor solution, CdO (123 mg), OA (2.45 ml), and ODE (10.8 ml) were placed in a flask and degassed under vacuum at 100 °C for 1 hour. The temperature was then raised to 250 °C under a nitrogen flow and maintained for 1 hour, until a clear solution formed. The precursor solution was cooled to 100 °C and held at that temperature until it was injected during CdS-shell growth.
The TOP-S precursor solution was prepared by stirring TOP (18 ml) and sulfur powder (44.3 mg) overnight in a glovebox.
For shell growth, Mn-doped CdSe quantum dots (75 mg) were dissolved in a mixture of ODE (28 ml), OAm (2.4 ml), and OA (1.2 ml). The mixture was degassed under vacuum at 100 °C for 1 hour. Under a nitrogen flow, the flask was heated to 220 °C. Aliquots of the Cd oleate and TOP-S precursor solutions, 0.4 ml each, were then injected dropwise and alternately for two cycles, with a 2.5-minute interval between injections.
Manufacture of Auston-switch devices
A 100 nm gold layer was deposited on the back side of a 1 mm glass substrate to serve as a ground plane. Films approximately 200 nm thick, consisting of either undoped reference quantum dots or Mn-doped CdSe/CdS quantum dots, were deposited on the top surface through repeated spin-coating cycles involving ligand exchange and rinsing. The quantum dots were dispersed in octane at 20 mg ml−1 and spin-coated at 1,600 rpm for 30 seconds.
To facilitate charge transport between quantum dots, the original long-chain ligands were replaced through solid-state ligand exchange with short, bifunctional 1,2-ethanedithiol (EDT) molecules. For each exchange step, 60 μl of a 1 M EDT solution in methanol (MeOH) was dropped onto the quantum-dot layer, allowed to soak for 60 seconds, and then spin-coated for 30 seconds at 1,200 rpm.
The film was subsequently rinsed with pure MeOH by spin-coating to remove excess ligand. The three steps—quantum-dot deposition, ligand exchange, and rinsing—were repeated five times to produce a quantum-dot layer approximately 200 nm thick. The resulting film was annealed at 150 °C for 30 minutes.
Finally, two 200 nm-thick gold contacts separated by a 70 μm gap were deposited on top of the quantum-dot film through a shadow mask. Together with the gold ground plane on the back of the substrate, the contacts formed a microstrip transmission line with a nominal impedance of 50 Ω.
To verify that ligand exchange and film fabrication preserved the quantum-confined electronic structure of the quantum dots, additional TA measurements were performed on a 200 nm-thick Mn-doped CdSe/CdS quantum-dot film prepared using the same ligand-exchange procedure as the TPC device. The membrane samples were analyzed under identical excitation conditions: 3.6 eV excitation, 150 fs pulse duration, and an average excitation number of N = 0.3. The results are shown in Extended Data Figure 8.
Equilibrium electrical properties were characterized through additional dark-conductivity measurements. A 120 nm-thick Mn-doped CdSe/CdS quantum-dot film was deposited on a glass substrate in contact with thermally deposited interdigitated Au electrodes. The electrodes contained 25 pairs of 2 mm-long fingers separated by 10 μm spacing. The corresponding current-voltage characteristics are shown in Extended Data Figure 2.
Electrostatic simulations of the Auston-switch geometry were performed using the electrostatic interface in COMSOL Multiphysics to calculate the electric-field distribution, effective gap capacitance, and effective RC constant. The results are shown in Extended Data Figure 1.
Transient-absorption measurements
TA measurements were performed using a standard pump-probe setup. In this arrangement, short pump pulses induced absorption changes that were measured in both the time and spectral domains using probe pulses with variable delays. The TA system was based on a regeneratively amplified ytterbium-doped potassium tungstate gadolinium (Yb:KGW) femtosecond laser (PHAROS, Photoconversion), which generated approximately 190 fs pulses at 1.2 eV.
The laser output was split into two beams. One beam seeded a harmonic generator (HIRO HHG, Photoconversion) to produce second-harmonic (2.4 eV) or third-harmonic (3.6 eV) pump pulses. Nonlinear optical pulse compression shortened these pulses to approximately 150 fs. Pulses from the second beam were delayed relative to the pump using an optical delay line with a range of up to 5 ns. They were focused onto a 3 mm-thick sapphire plate to generate broadband probe pulses in the form of a femtosecond white-light continuum.
The pump beam was focused on the sample to a spot approximately 120 μm in diameter. The smaller probe beam, with a diameter of less than 90 μm, was focused near the center of the pump spot. Probe pulses transmitted through the sample were detected with an Avantes AvaSpec-Fast ULS1350F-USB2 spectrometer. The measured TA spectra were corrected for chirp—the wavelength-dependent delay within the white-light continuum—using the procedure described in Ref. 2
In Auger-recombination studies of undoped and manganese-doped quantum dots, pump-induced bleaching of the band-edge absorption, Δα, was used to track the decay of the exciton population at the band edge.14
TPC measurements
To minimize sample degradation during TPC measurements, the fabricated Auston-switch device was mounted in a nitrogen-filled, airtight chamber equipped with an optical window and electrical feedthroughs. No measurable changes in the TPC response were observed during the full device characterization, including measurements dependent on pump fluence, transport distance, and applied bias.
The chamber was mounted on a translation stage, allowing the laser-beam position within the electrode gap to be varied. One of the top gold electrodes was biased with a DC power supply (Keithley 2430), while the other was connected by coaxial cable to a 20 GHz-bandwidth sampling oscilloscope. To reduce timing jitter, the oscilloscope was triggered by an electrical pulse from a fast Si photodetector illuminated by a portion of the laser beam split from the excitation path.
The quantum dots in the Auston-switch photoconductive gap were excited at 2.4 eV or 3.6 eV with 150 fs pulses from the second or third harmonic, respectively, of an amplified Yb:KGW femtosecond PHAROS laser. A cylindrical achromatic lens focused the laser beam into a narrow stripe along the edge of the top gold electrode. Beam-profiler measurements showed that the excitation profile was approximately Gaussian, with a stripe width of approximately 70–80 μm full width at half maximum (FWHM).
The excitation position within the photoconductive gap was varied by moving the sample in a plane perpendicular to the laser beam. The position was initially calibrated with a beam profiler and monitored in real time on the sample using a CMOS camera.
As discussed in Supplement 3, the nonlinear dependence of SE-Auger upconversion on excitation density produces a narrower lateral spatial profile for the mobile hot-electron population than for the laser beam itself, as shown in Extended Data Figure 9. Across the film thickness, the initial hot-electron population was weighted toward the irradiated surface. However, because the optical absorption length was comparable to the quantum-dot film thickness, excited Mn ions were generated throughout the layer. Consequently, SE-Auger regeneration remained active across the film thickness, even though the hot-electron population spread vertically while traveling through the photoconductive gap.
Source: www.nature.com